Reproduce a Saturated Iron Glaze
cone 10 oxidation
Firing profile
A two hour hold at 1850 deg F
A half hour hold at 1750 deg F
A three hour hold at 1700 deg F
slow downfire at 25 deg F an hour in the interval 1700 deg F to 1650 deg F
A half hour hold at 1650 deg F
Clay body is a grolleg porcelain from Tacoma Clay Art Center.
In Previous Firings
Glazes were seen previously in a different firing in the same kiln with the
same firing protocol.
Leaf One
Leaf Two
The pots are pasta bowls ~11 inches in diameter.
glaze satIron_ZG_H_0
glaze satIron_ZG_H_5
glaze satIron_ZG_0