Interactions of Viscous glazes

This is a further exploration of a firing which has a slow up-fire in addition to having the usual
holds on the way down.

The matrix glaze, hiAlk_satIron_Z4L_0MCa, is on the edge of fully matured. It is covered in
micro-crystalline clusters separated from each other by lines of pits.

The inlay glaze, hiAlk_Z3P_M_hAlk, with slightly higher silica, is smoother and does not have the visible
pinholes of the matrix glaze. Both the inlay and matrix glaze have high viscosity, and a
large volume of crystals.

As a result of this, the interaction region is comprised of small shapeless masses with distinct components
of the two glazes. Tendrils of matrix glaze infiltrate the inlay, maintaining their own identity.

The color of the glaze shifts from pale green through yellow, then orange to a vivid red-orange as the
thickness of the glaze increases.

The matrix (i.e., background) glaze and inlay glaze overlap minimally before firing. The width of the
original inlay varied from an eighth of an inch to three quarters of an inch.

The design is created by adhering a mask and then applying the main glaze. After drying,
emulsion wax is applied, the mask is removed and the open area filled in with a second glaze,
using an ear syringe.

The close-up images were heavily edited to enhance detail. The colors of the full image of the bowl
are as they appear in bright light.



Close up Images of the interaction region

full view

full view

full view

full view

full view



Image of the piece

full view

full view

bowl with glaze hiAlk_satIron_Z4L_0MCa and inlay hiAlk_Z3P_M_hAl_lSi

bowl is ~6 inches in diameter



oxidation firing to a hot cone 10 in an electric kiln

Firing profiles

Up Fire profile hot cone 10

400 deg F an hour to 1800 deg F

300 deg F an hour to 2050 deg F

200 deg F an hour to 2240 deg F then a 90 min hold at 2240 deg F

90 deg F an hour to 2320 deg F

Down Fire Profile hot cone 10

300 deg F an hour to 1850 deg F then a 2 hr hold at 1850 deg F

300 deg F an hour to 1750 deg F then a 1 hr hold at 1750 deg F

300 deg F an hour to 1700 deg F then a 3 hr hold at 1700 deg F

25 deg F an hour to 1650 deg F then a 1 hr hold at 1650 deg F



Clay body is a grolleg porcelain from Clay Art Center in Tacoma, WA.



glaze composition

Empirical Formula hiAlk_satIron_Z4L_0MCa :

K2O        0.12
Na2O       0.45
CaO        0.42
MgO        0.01

Al2O3      0.62
Fe2O3      0.10

SiO2       3.0
P2O5       0.06
TiO2       0.11

molecular percent Silica 61.4%



Inlay Glaze:

Empirical Formula hiAlk_Z3P_M_hAl_lSi

K2O        0.12
Na2O       0.50
CaO        0.36
MgO        0.02

Al2O3      0.64

SiO2       3.66
P2O5       0.07
TiO2       0.22

ppp molecular percent Silica 65.6%



Remarks

This firing features a 'rounded at the top' firing profile; with a hold of an hour and a half at 80 degreesF
below top temperature, and a slow climb from there to the top temperature.