Interactions in a high titanium glaze

This is a further exploration of a firing which has a slow up-fire in addition to having the usual
holds on the way down.

Here is another in the series of high titanium glazes, which I'd called snowflake glazes for
the snowflake-like clusters of titanium crystals that occasionally grow in these glazes.

The inlay glaze, oribe-woof-black-M is seen here.

The matrix glaze, hiAlk_Z3P_M_hAl_lSi, is a cousin of the glaze seen in the above
note, it has higher alumina and silica, and a higher silica:alumina ratio as well. It is a more
viscous glaze.

The structure of the interaction region is strikingly different as a result of these shifts in the
chemistry of the inlay glaze. The large titanium crystal clusters which had been seen in the prior
note are gone. The distinctive sharply-demarcated band of copper which had diffused into the
matrix glaze is replaced by a dispersion of particles far into the matrix, but nowhere is it dense.

The matrix (i.e., background) glaze and inlay glaze overlap minimally before firing. The width of the
original inlay varied from an eighth of an inch to three quarters of an inch.

The design is created by adhering a mask and then applying the main glaze. After drying,
emulsion wax is applied, the mask is removed and the open area filled in with a second glaze,
using an ear syringe.

The close-up images were heavily edited to enhance detail. The colors of the full image of the bowl
are as they appear in bright light.



Close up Images of the interaction region

full view

full view

full view

full view

full view

full view



Image of the piece

full view

bowl with glaze hiAlk_Z3P_hAl_lSi and inlay glaze oribe-woof-black-M

bowl is ~6 inches in diameter



oxidation firing to a hot cone 10 in an electric kiln

Firing profiles

Up Fire profile hot cone 10

400 deg F an hour to 1800 deg F

300 deg F an hour to 2050 deg F

200 deg F an hour to 2220 deg F then a 90 min hold at 2240 deg F

90 deg F an hour to 2320 deg F

Down Fire Profile hot cone 10

300 deg F an hour to 1850 deg F then a 2 hr hold at 1850 deg F

300 deg F an hour to 1750 deg F then a 1 hr hold at 1750 deg F

300 deg F an hour to 1700 deg F then a 3 hr hold at 1700 deg F

25 deg F an hour to 1650 deg F then a 1 hr hold at 1650 deg F



Clay body is a grolleg porcelain from Clay Art Center in Tacoma, WA.



glaze composition

Empirical Formula hiAlk_Z3P_M_hAl_lSi

K2O        0.12
Na2O       0.50
CaO        0.36
MgO        0.02

Al2O3      0.64

SiO2       3.66
P2O5       0.07
TiO2       0.22

molecular percent Silica 65.6%



Inlay Glaze:

Empirical Formula oribe-woof-black-M

K2O        0.10
Na2O       0.04
CaO        0.69
MgO        0.17

Al2O3      0.38

SiO2       3.15
P2O5       0.01
ZrO2       0.05

molecular percent Silica 68.4%

Added:

5.0% Copper Oxide
0.75% Cobalt Carbonate



Inlay Glaze:

Remarks

This firing features a 'rounded at the top' firing profile; with a hold of an hour and a half at 100 degreesF
below top temperature, and a slow climb from there to the top temperature.

Carol's Home Page