Interactions of Low Viscosity glazes

This is a further exploration of a firing which has a slow up-fire in addition to having the usual
holds on the way down.

The matrix glaze, hiAlk_atIron_Z4L_0MCa_PSi, with high alumina and even higher alkali metals has low
viscosity, yet is pinned in place by clusters of rutile crystals. The inlay glaze, oribe-woof-black-M, with
a high silica:alumina ratio has lower alkali metals, so has low viscosity with sufficient surface
tension to stay put. The inlay glaze contains zirconium which also crystallizes.

The interaction region surrounding the inlay is covered in flat needle crystals which form
clusters of acicular micro-crystals. These crystals detach from this border, migrating both into the matrix
glaze and the inlay glaze.

The matrix (i.e., background) glaze and inlay glaze overlap minimally before firing. The width of the
original inlay varied from an eighth of an inch to three quarters of an inch.

The design is created by adhering a mask and then applying the main glaze. After drying,
emulsion wax is applied, the mask is removed and the open area filled in with a second glaze,
using an ear syringe.

The close-up images were heavily edited to enhance detail. The colors of the full image of the bowl
are as they appear in bright light.



Close up Images of the interaction region



Image of the piece

full view

full view

bowl with glaze hiAlk_satIron_Z4L_0MCa_PSi and inlay glaze oribe-woof-black-M

bowl is ~6 inches in diameter



oxidation firing to a hot cone 10 in an electric kiln

Firing profiles

Up Fire profile hot cone 10

400 deg F an hour to 1800 deg F

300 deg F an hour to 2050 deg F

200 deg F an hour to 2240 deg F then a 90 min hold at 2240 deg F

90 deg F an hour to 2320 deg F

Down Fire Profile hot cone 10

300 deg F an hour to 1850 deg F then a 2 hr hold at 1850 deg F

300 deg F an hour to 1750 deg F then a 1 hr hold at 1750 deg F

300 deg F an hour to 1700 deg F then a 3 hr hold at 1700 deg F

25 deg F an hour to 1650 deg F then a 1 hr hold at 1650 deg F



Clay body is a grolleg porcelain from Clay Art Center in Tacoma, WA.



glaze composition

Empirical Formula hiAlk_satIron_Z4L_0MCa_PSi :

K2O        0.12
Na2O       0.45
CaO        0.42
MgO        0.01

Al2O3      0.63
Fe2O3      0.11

SiO2       3.46
P2O5       0.07
TiO2       0.12

molecular percent Silica 64.3%



Inlay Glaze:

Empirical Formula oribe-woof-black-M

K2O        0.10
Na2O       0.04
CaO        0.69
MgO        0.17

Al2O3      0.38

SiO2       3.15
P2O5       0.01
ZrO2       0.05

molecular percent Silica 68.4%

Added:

5.0% Copper Oxide
0.75% Cobalt Carbonate



Remarks

This firing features a 'rounded at the top' firing profile; with a hold of an hour and a half at 80 degreesF
below top temperature, and a slow climb from there to the top temperature.

Carol's Home Page